Case studies / New energy vehicle battery sealing

Battery pack seal: VOC compliance without losing compression set

A peroxide-to-addition conversion on a battery pack seal, where VOC compliance and compression set had to be met in the same production trial.

New energy vehicle battery sealingEncapsulationPC-12
Result at a glance
+40%
cell uniformity
8%
compression set, down from over 10%
VOC-free
addition cure, no by-products

Each figure is tied to a measurement, and the result section below states the conditions that produced it. Field data and accelerated aging data are labelled separately, and the disclosure at the end of the case states how the data was obtained.

Visualised

Measured, not claimed.

Schematic of the measurement behind this case: the same conditions, drawn to be read at a glance. The drawing is illustrative; the measured values are the ones stated in the result sections.

Cure kinetics with and without PC-611 inhibitorCURE KINETICS · SCHEMATIC · 100 °C CURE STEP02550751000TIMECURE DEGREE (%)100 °C CURE STEPno inhibitorwith PC-611steep risePOT LIFE AT ROOM TEMPERATURE (HOURS TO ONE WEEK)
Schematic cure kinetics, not measured data: PC-611 holds the mixed batch workable at room temperature, then cure rises steeply once the part reaches the 100 °C cure step. Read it as a comparison of curve shapes, not as a rate table.
01 / Challenge

The challenge.

A battery pack seal was built on a peroxide cure system. VOC emissions failed the customer's incoming specification, and the alternative addition-cure trial produced uneven cell structure and compression set above the 10% limit.

Both failures had to be closed at once. A seal that cures evenly but sets too hard still leaks, and a seal that is soft enough but emits volatiles does not pass incoming inspection. The trial therefore had to fix cure uniformity and compression set together, in a section thick enough for cure gradients to matter.

The peroxide system also set the baseline for compression set, which is why the first addition-cure trial was judged against a 10% limit. That limit, not the VOC result, is what the alternative system failed.

02 / Solution

The solution.

5,000 PPM platinum catalyst at 0.08% dosage, with PC-611 inhibitor to keep the mixed batch workable for the potting window.

Platinum loading set the cure speed through the section; the inhibitor set how long the batch stayed usable before the pour. The dosage was kept in the lower half of the 0.05%–0.5% range: enough activity for the section, without pushing the cure so fast that the batch gelled in the mix head.

Because the system is addition-cure, no peroxide by-products are released during cure. That is the mechanism behind the VOC result, and it is a property of the chemistry rather than of a post-cure treatment.

03 / Result

The result, and what produced it.

The numbers at the top of the page are the headline metrics from this case. The paragraphs here explain what produced them, with the test method and the exposure stated alongside.

Cell uniformity improved by 40% against the failed trial, and compression set came in at 8% — below the 10% limit the first addition-cure trial exceeded. Compression set was measured per the customer's internal method after 24 h at 100°C, and cell structure was read from a cured section.

The two numbers answer different questions: uniformity describes how the section cured, compression set describes how the seal behaves in service. A formulation change that improves one can move the other, which is why both are reported.

The figures describe this seal geometry, this section thickness and this cure schedule. A different section or a different contamination profile should be re-trialled rather than scaled from these numbers.

Test conditions and data scope

Customer production line trial; cell structure measured on cured section, compression set per customer internal method after 24 h at 100°C.

Customer production case, published with permission and without customer identification.

Traceability

The grades and the application behind this case.

Every case is tied to a catalyst grade and to an application page. The grade page carries the full specification; the application page carries the process window, dosage range and inhibitor pairing for this class of part.

ModelPt concentrationViscosityRecommended dosage
PC-125,000 PPM400–500 cP0.05%–0.5% of total compound

Open a model for packaging, shelf life, features and inhibitor pairing. Where a case names more than one grade, the solution section states which one was used in the reported trial.

Application

Encapsulation

Stable cure where the chemistry fights back.

Anti-poisoning catalysis for potting, encapsulation and high-voltage insulation, where contaminants and thick sections defeat ordinary catalysts.

PC-18BPC-18APC-50
Next step

Run a comparable trial on your own line.

Send the part, the failure and the acceptance test. We will send evaluation samples of the grade used in this case, paired with the matching inhibitor, and confirm the starting dosage for your cure window.

Technical reply within 24 hours
Evaluation samples in 5–7 days
COA, TDS and SDS on request
Custom concentration 1,000–20,000 PPM